Aug 09, 2023 Kite yon mesaj

Sb Doped O3 Kalite Na0.9Ni0.5Mn{0.3Ti0.2O2 Katod Materyèl Pou Na-ion Battery

KONG Guoqiang, LENG Mingzhe, ZHOU Zhanrong, XIA Chi, SHEN Xiaofang. Sb Doped O3 Kalite Na0.9Ni0.5Mn0.3Ti0.2O2 Katod Materyèl pou Na-ion Battery[J]. Journal of Inorganic Materials, 2023, 38(6): 656-662.

 

Résumé


Estabilite sik ak kapasite espesifik materyèl katod pou pil ion sodyòm jwe yon wòl enpòtan nan reyalize aplikasyon lajè yo. Baze sou estrateji pou entwodwi heteroelements espesifik pou optimize estabilite estriktirèl la ak kapasite espesifik materyèl katod, O{{0}}Na0.9Ni0.5-xMn 0.3Ti0.2SbxO2 (NMTSbx, x{{10}}, 0.02, {{20 }}.04, 0.06) te prepare pa yon senp metòd reyaksyon eta solid, ak efè kantite dopan Sb sou pwopriyete depo sodyòm Na{{46 }}.9Ni0.5Mn{{50}}.3Ti0.2O2 materyèl katod yo te envestige. Rezilta karakterizasyon yo montre ke fòs repouse elektwostatik ant atòm oksijèn nan kouch metal tranzisyon an redwi apre Sb dopaj, pandan y ap espas lasi a elaji, ki se fezab deintercalation nan Na plis. Pandan se tan, delokalizasyon nan elektwon fò ki te koze pa Sb dopan diminye enèji nan tout sistèm nan, ki mennen ale nan yon estrikti ki estab, plis fezab nan chaje siklik ak egzeyat. Tès elektwochimik la montre ke inisyal egzeyat espesifik kapasite NMTSb0 undoped se 122.8 mAh·g-1 nan 1C (240 mA·g-1), ak pousantaj la retansyon kapasite se sèlman 41.5 pousan apre 200 sik. Men, premye egzeyat kapasite espesifik nan dope NMTSb0.04 se 135.2 mAh·g-1 nan 1C, ak pousantaj retansyon kapasite a se jiska 70 pousan apre 200 sik. Etid sa a montre ke Sb dope O3 kalite Na0.9Ni0.5Mn0.3Ti0.2O2 katòd materyèl ka siyifikativman amelyore egzeyat inisyal kapasite espesifik ak pousantaj retansyon kapasite nan pil ion sodyòm. Rezilta nou yo sijere ke estrateji dopaj Sb ta ka yon apwòch itil pou preparasyon pil iyon sodyòm ki estab ki wo.

 

Mo kle:Sb dopaj; O3 kalite; materyèl katod; metòd faz solid; vòltaj lajè; Na-ion batri

 

Depi komèsyalizasyon pil ityòm-ion yo, yo te lajman itilize nan aparèy elektwonik pòtab, machin elektrik ak depo enèji elektwochimik, elatriye. Sepandan, resous yo limite ak distribisyon inegal nan ityòm se yon faktè enpòtan mete restriksyon sou devlopman nan ityòm-ion pil. . An menm tan an, rezèv sodyòm yo abondan ak lajman distribiye, ak pi enpòtan, akòz resanblans nan pwopriyete chimik ityòm ak sodyòm, prensip k ap travay nan pil sodyòm-ion se tou pre sa yo ki nan ityòm-ion pil. Se poutèt sa, aplikasyon an nan pil sodyòm-ion nan jaden an nan gwo-echèl depo enèji te resevwa gwo atansyon.

Materyèl katod pou pil sodyòm-ion sitou gen ladan metal tranzisyon kouch oksid, konpoze polianionik, ak analogue Prussian ble. Pami yo, oksid kouch NaxTMO2 (TM refere a metal tranzisyon, 0

Pami divès kalite O{{0}}materyèl NaxTMO2 ki te rapòte, NaxTMO2 ki gen Ni ak Mn te atire anpil atansyon poutèt resous Ni/Mn abondan li yo ak gwo kapasite depo. Pa egzanp, O3-tip NaNi0.5Mn0.5O2 gen yon gwo kapasite revèsib (133mAh g-1). Bon pèfòmans pousantaj (30C, 40mAh g-1) ak lavi sik long (70 pousan retansyon kapasite espesifik apre 500 sik nan 3.75C). Sepandan, toujou gen kèk pwoblèm ki mete restriksyon sou devlopman pi lwen li yo, tankou pèfòmans pousantaj ki pa satisfezan, tranzisyon faz konplèks pandan chaj ak egzeyat, ak pouri kapasite rapid espesyalman nan vòltaj segondè nan 4.1-4.5 V. Dènye etid yo te montre ke pasyèl dopaj nan lòt eleman. ka efektivman amelyore revèsib tranzisyon faz la. Pou egzanp, Ti-dope Na0.9Ni0.4Mn0.4Ti0.2O2 gen yon tranzisyon faz O3-P3 ki pi revèsib ant 2.5 ak 4.2 V, pi wo kapasite espesifik (197 mAh g{{39} }), ak pèfòmans sik ki pi estab. Fe-dope NaFe0.2Mn0.4Ni0.4O2 gen yon gwo kapasite revèsib (165 mAh g-1) ak yon tranzisyon faz ki estab (87 pousan retansyon kapasite apre 200 sik) nan seri a nan 4.0-4 .3 V.

Anplis de sa, Sb5 plis dopaj kapab tou amelyore estabilite sik la ak vòltaj k ap travay nan materyèl katod. Yo nan lòd yo jwenn yon estrikti materyèl ki pi estab ak pèfòmans pousantaj siperyè nan yon ranje vòltaj pi laj pou O3-kalite oksid kouch. Nan etid sa a, Sb5 plis te pasyèlman ranplase Ni2 plis nan Na0.9Ni0.5Mn{0.3Ti0.2O2 (NMT) pa yon senp solid- metòd leta pou etidye efè Sb dopaj sou pèfòmans elektwochimik kouch oksid ak chanjman revèsiblite tranzisyon faz O3-P3 nan yon ranje vòltaj lajè.

 

1 Metòd eksperimantal


 

1.1 Preparasyon materyèl

Na{{0}}.9Ni0.5-xMn0.3Ti{{1{0}}.2SbxO2 (NMTSbx, x{{9 }}, 0.02, 0.04, 0.06) materyèl yo te prepare pa metòd faz solid. Etap espesifik yo se jan sa a: melanje Na2CO3, NiO, Sb2O5, MnO2, ak TiO2 nan rapò esteyyometrik ki koresponn lan, epi ajoute yon lòt 5 pousan fraksyon mol Na2CO3 an konsiderasyon volatilité Na nan tanperati ki wo. Moulen li respire ak yon mòtye agat epi sèvi ak yon machin tablèt pou fè yon disk mens ϕ16 mm. Tretman chalè nan 950 degre nan atmosfè lè de fwa, chak fwa pou 12 h. Menm pwosedi a te itilize pou prepare NMTSb0 san Sb2O5 kòmanse materyèl, ak tout echantiyon yo te estoke nan yon bwat gan pou itilize nan lavni.

 

1.2 Asanble batri

Materyèl aktif NMTSbx, asetilèn nwa ak fliyò polyvinylidene (PVDF) yo te peze nan yon rapò mas 7:2:1, epi yo te ajoute yon kantite apwopriye nan N-methylpyrrolidone (NMP) pou moulen pou jwenn yon sispansyon melanje inifòm. Sispansyon an te kouvwi sou sifas papye aliminyòm, epi chaje sifas materyèl aktif nan elektwòd la te apeprè 2.5 mg cm -2. Vacuum-seche nan 80 degre pou 12 èdtan, ak Lè sa a, koupe an ti disk nan ϕ12 mm ak yon mikrotom kòm elektwòd pozitif la. Selil bouton CR2032 yo te rasanble nan yon bwat gan ki te ranpli avèk gaz Ar (fraksyon volim dlo ak oksijèn yo te pi ba pase 1×10-6). Pami yo, elektwòd vann san preskripsyon an se fèy metal sodyòm, separasyon an se fib vè, ak elektwolit la se 1 mol L-1 NaClO4 dibutil carbonate plis solisyon fluoroethylene carbonate (rapò volim 1: 1).

 

1.3 Materyèl Karakterizasyon ak Tès

Yo te teste spectre difraksyon radyografi (XRD) echantiyon an lè l sèvi avèk MiniFlex 600 (Rigaku, Japon, Cu K ), epi Rietveld te rafine estrikti kristal la atravè sistèm analiz estriktirèl la (GSAS plis EXPGUI). ). Mòfoloji mikwoskopik ak gwosè patikil echantiyon yo te obsève pa JSM-7610F (JEOL, Japon) mikwoskòp elèktron (SEM) ak JEOL JEM-2100F mikwoskòp elèktron transmisyon segondè rezolisyon (HRTEM). X-ray photoelectron spectroscopie (XPS) nan eta a valans nan eleman yo te teste sou yon espektwomèt Escalab250xi lè l sèvi avèk AlK achromatik X-ray sous. Yo te analize rapò molè chak eleman nan echantiyon an pa espektwomèt emisyon optik plasma ki makonnen endiktif (ICP-AES, iCAP 6300). Mezi chaj ak egzeyat yo te fèt nan tanperati chanm lè l sèvi avèk yon sistèm tès batri Land CT2001A ant 2.0 ak 4.2 V, epi yo te mezire espektroskopi elektwochimik enpedans (EIS) elektwòd yo lè l sèvi avèk yon estasyon elektwochimik CHI660E (CH Instruments).

 

2 Rezilta ak diskisyon


2.1 Karakteristik estriktirèl nan NMTSbx

Konpozisyon elemantè tout echantiyon yo te detèmine pa ICP-AES, epi rezilta yo montre nan Tablo S1. Nan seri erè mezi, kontni aktyèl la nan chak ion metal se fondamantalman ki konsistan avèk konpozisyon konsepsyon an. Nan spectre XRD nan Fig. 1(a), tout echantiyon yo genyen estrikti O3-tip egzagonal -NaFeO2 (gwoup espas R-3m), ki konsistan avèk NaNi0.5Mn{{ 9}}.5O2 (JCPDS 54-0887). Li montre ke entwodiksyon Sb nan lasi NMT a pa chanje estrikti intrinsèques materyèl la. Pwosesis pou prepare katod oksid segondè-nikèl kouch pa metòd solid-eta a pral inevitableman pwodwi yon ti kantite eleman rezidyèl NiO inaktif, ak literati a montre ke enpak la nan kantite tras nan NiO sou pèfòmans batri se neglijab. Nan Fig. 1(b), pik difraksyon NMTSb0.02, NMTSb{{{20}}.04, ak NMTSb{{28 }}.06 te deplase nan gwo ang, ak pik divès te kòmanse parèt nan NMTSb0.06. Dapre ekwasyon Bragg (nλ=2dsinθ), gwosè mwayèn grenn poud lan analize kalitatif. kote n se lòd difraksyon an, d se epesè mwayèn (nm) grenn echantiyon an pèpandikilè ak direksyon plan kristal la, θ se ang difraksyon ki koresponn ak pik difraksyon ki pi fò a, ak λ se radyografi a. longèdonn (nm). Rezilta kalkil avyon kristal yo montre ke gwosè grenn echantiyon an diminye apre Sb dopaj, ki gen rapò ak diferans ki genyen nan reyon iyonik Sb (0.06 nm) ak Ni (0.069 nm). Dapre teyorèm Vegard a, sa vle di tou ke yon reyaksyon solisyon solid te fèt pandan fòmasyon NMTSbx.

Na-ion Battery Cathode Material

Fig. 1 Sondaj (a) ak elaji (b) modèl XRD nan NMTSbx (x=0, 0.02, 0.04, 0.06)

 

Figi 2 (a, b) montre modèl XRD Rietveld rafine NMTSb0 ak NMTSb{0.04, ak paramèt lasi detaye yo montre nan Tablo S2. Ou ka wè paramèt lasi NMTSb{{10}}.04 (a=b{=0.2979{{20 }} nm) yo yon ti kras redwi konpare ak orijinal NMTSb0 (a=b{=0.29812 nm). Sa a tou atribiye a lefèt ke reyon iyonik Sb (0.06 nm) pi piti pase sa ki nan Ni (0.069 nm), ki se ki konsistan avèk analiz XRD la. C (c=1.608391 nm) nan NMTSb0.04 te ogmante konpare ak sa yo ki nan NMTSb0 (c=1.600487 nm). Rezon prensipal ki fè se ke paramèt lasi a / b a sansib a chanjman nan longè kosyon (Ni / Mn / Ti / Sb) -O nan plan an fondamantal estrikti kouch, ak enkòporasyon an nan Sb rakousi longè kosyon an. Sa lakòz repouse elèktrostatik ant atòm oksijèn nan kouch metal tranzisyon kontinyèl (Ni/Mn/Ti/Sb) vin pi gwo, ki mennen nan yon ogmantasyon nan c. Anplis, apre kalkil, c / a nan NMTSb0 ak NMTSb0.04 pa t 'chanje anpil, yo te 5.36 ak 5.39 respektivman, tou de te pi gran pase 4.99, ki endike ke echantiyon yo doped kenbe yon bon estrikti kouch.

Na-ion Battery Cathode Material

Fig. 2 Modèl XRD rafineman Rietveld nan NMTSb0 (a) ak NMTSb0.04(b)

 

Figi 3 montre foto SEM NMTSb0 ak NMTSb0.04. Tou de pwodwi yo konpoze de yon gwo kantite mikwo-nano-echèl disk mens ak epesè inifòm ak bor klè. Espesyalman apre Sb dopaj, sifas flak la pi dous, epi pa gen okenn mank de estrikti flak egzagonal ak kwen byen file ak kwen. Analiz elemantè EDS nan zòn chwazi nan NMTSb0.04 montre ke eleman Na, O, Ni, Ti, Mn, ak Sb yo distribye egalman nan echantiyon an, ki pwouve tou ke eleman Sb yo te dope avèk siksè nan intrinsèque la. estrikti nan NMTSb0.

Na-ion Battery Cathode Material

Fig. 3 Imaj SEM ak kat EDS nan NMTSb0 (a, b) ak NMTSb0.04 (c, d)

 

HRTEM te obsève mikrostruktur NMTSb{{0} ak NMTSb0.04, e rezilta yo montre nan Figi S1. Nan Figi S1 (a, c), patikil yo anvan ak apre dopaj Sb yo konekte oswa sipèpoze, ak makroskopik parèt kòm yon estrikti ki sanble ak fèy oswa apeprè sikilè oswa poligonal. Imaj HRTEM nan Figi S1(b, d) montre fwontyè lasi materyèl la, ak espas lasi NMTSb{{10}} ak NMTSb0.04 yo. 0.238 ak 0.237 nm, respektivman. Tou de koresponn ak (101) kristal avyon an, ak efè dopan Sb sou espas lasi a konsistan avèk rezilta analiz XRD yo. Ensèk yo nan Figi S1 (b, d) yo se tach yo nan modèl la diffraction elèktron zòn chwazi (SEAD) nan NMTSb0 ak NMTSb0.04, ki pwouve ke NMTSb0 yo jwenn ak NMTSb0.04 gen bon kristalinite.

 

Spectroskopi fotoelectron radyografi (XPS) Figi S2 montre rezilta eta oksidasyon eleman Mn, Ni, Ti, ak Sb nan NMTSb0 ak NMTSb0.04. Nan Figi S2(a), de pik prensipal NMTSb0 nan 877 ak 850 eV koresponn ak Ni2p1/2 ak Ni2p3/2, respektivman, epi tou de fè pati Ni2 plis nan echantiyon an. Pik enèji obligatwa nan 858.2 eV se yon pik satelit komen nan eleman Ni. Ni2p1/2 nan NMTSb0.04 divize an de pik, sa ki endike ke entwodiksyon Sb nan lasi NMTSb0 ka diminye kantite elektwon deyò alantou Ni, sa ki lakòz yon efè delokalizasyon elèktron fò. Metal tranzisyon yo gen plis delokalize d orbitals, sa ki ka amelyore entèraksyon metal-metal nan oktaèd MO6 pataje bò nan estrikti a kouch, kidonk anpeche efondreman nan oktaèd MO6 ak soulaje reyaksyon segondè nan oksijèn lasi ak elektwolit. Pandan pwosesis chaj-egzeyat la, estrikti materyèl la oksid kouch vin pi estab, sa ki endike ke fò delokalizasyon elèktron benefisye estabilite estriktirèl NMTSb0.04. Pou eleman Mn, pik Mn2p3/2 nan 642 eV ak pik Mn2p1/2 nan 652 eV nan Figi S2(b) endike prezans Mn nan eta valans plis 4 nan tou de NMTSb0 ak NMTSb{ {84}}.04. Mn2p3/2 pik la nan 643eV ka matche ak pik Mn3 plis la. Konfigirasyon oktaedrik Mn3 plis yo pral defòme, ki se koze pa distòsyon jenjanm-Taylor. Disolisyon nan eleman Mn ap mennen nan yon bès rapid nan kapasite, pandan y ap Ti nan NMTSb0.04 ranplase yon pati nan Mn, ak rediksyon nan kontni Mn kapab tou estabilize fondasyon an estriktirèl nan materyèl la, kidonk anpeche n bès rapid nan kapasite batri ki te koze. pa efè jenjanm-Taylor. Tipik pik enèji obligatwa Ti2p1/2 ak Ti2p3/2 nan 457.3 ak 453.1 eV pou NMTSb0 nan Figi S2(c) koresponn ak eta a ki estab plis 4 valans nan Ti. Pandan ke Ti2p1/2 ak Ti2p3/2 pik nan 454.1 ak 463.9 eV nan NMTSb0.04 koresponn ak Ti nan eta a valans plis 3. Soti nan pèspektiv nan konpansasyon chaj, sa a se sitou akòz reyaksyon an rediksyon nan Ti apre entwodiksyon nan wo-valans Sb5 plis . Pandan reyaksyon chaj-egzeyat la, Ti4 plis kontinye egziste nan yon fòm ki estab, ki te verifye nan koub voltametrii siklik (CV) nan NMTSb0.04, jan yo montre nan Figi 4. Sa a montre tou ke sous kapasite batri a pa gen anyen. fè ak pè Ti4 plis / Ti3 plis redox. Anplis de sa, pik enèji obligatwa NMTSb0.04 nan 529-536 eV nan Figi S2 (d) konfime prezans Sb.

Na-ion Battery Cathode Material

Figi 4 koub CV nan materyèl katod NMTSb0.04

 

2.2 Pèfòmans elektwochimik

Figi 5 montre enpedans elektwochimik Nyquist konplo NMTSbx la. Pami yo, demi sèk la nan rejyon an mwayen ak segondè frekans reprezante rezistans transfè chaj (Rct) ant elektwolit la ak elektwòd la, ak liy lan oblik nan rejyon an frekans ba reprezante rezistans nan Warburg ki te koze pa difizyon nan iyon sodyòm. Fikse sikwi ekivalan a montre ke Rct NMTSb0 ak NMTSb0.04 se 1185.4 ak 761 Ω, respektivman. Kòm kontni an dopaj Sb ogmante, enpedans echantiyon an diminye tou. Lè x=0.04, enpedans echantiyon an rive nan valè minimòm lan. Pli lwen ogmante kontni an dopaj Sb mennen nan yon ogmantasyon nan enpedans. Lè x=0.06, enpedans la depase echantiyon NMTSb0 la. Kontni dopan ki apwopriye ka jwenn espas entèrkouch metal pi bon nan estrikti a kouch, asire chanèl transpò elèktron lis, ede amelyore karakteristik sa yo dinamik nan NMTSb0.04, epi an menm tan an pran an kont estabilite nan estrikti an jeneral.

Na-ion Battery Cathode Material

Fig. 5 Spectre enpedans elektwochimik nan NMTSbx

 

Under the condition of current density of 1C (240 mA·g−1) and voltage range of 2.0-4.2 V, the sodium storage performance of the Na-ion battery with NMTSbx as the electrode was tested. As shown in Figure 6(a), the reversible capacities of NMTSbx (x=0, 0.02, 0.04, 0.06) samples are 122.8, 128.0, 135.2 and 103.9 mAh g−1, respectively. The difference in specific capacity is due to different doping content. The strategy of chemical element substitution can suppress the irreversible phase transition and improve the sodium ion transport kinetics. The advantages are summarized as follows: replace highly active elements with electrochemically inactive and structurally stable elements, such as preventing cation mixing by increasing the energy barrier of Ni2+ migration, and reducing the oxygen released during electrochemical cycling by strengthening metal-oxygen bonds. Doping or replacing transition metal sites can significantly inhibit the phase transition, inhibit transition metal ion migration, and improve the chemical and electrochemical stability of desodiumized materials. The specific doping content should be explored according to the type of doping element and the intrinsic structure. . On the one hand, doping with high-valent metal ions can improve the bulk conductivity of the material after the metal ions enter the interior of the lattice. When the mole fraction of doping is greater than 1% (stoichiometric ratio x>{{0}}.01), rezistivite a ap diminye rapidman, ki pral gen yon gwo enfliyans sou konduktiviti a. Nan lòt men an, kantite lajan dopan twò wo pral inevitableman redwi kontni an nan koup redox nan sistèm nan ak afekte dansite enèji nan sistèm nan, pandan y ap twò piti kantite dopan pa pral ase yo estabilize estrikti nan materyèl oksid kouch. Nan etid sa a, NMTSbx(x=0, 0.02, 0.04, 0.06), x se rapò esteyyometrik, ak kontni dopan aktyèl la se 2 pousan, 4 pousan ak 6 pousan pa fraksyon mol, respektivman.

Na-ion Battery Cathode Material

Fig. 6 Pèfòmans batri Na-ion ak NMTSbx kòm elektwòd

(a) Chaje ak dechaje koub batri Na-ion ak echantiyon kòm elektwòd pou premye sik la nan 1C; (b) Pèfòmans monte bisiklèt nan batri Na-ion ak echantiyon kòm elektwòd nan 1C pou 200 sik; (c, d) Chaje ak dechaje koub batri Na-ion ak echantiyon kòm elektwòd pou premye 3 sik nan 5C; (e) Efikasite koulombik batri Na-ion ak NMTSbx kòm elektwòd pou 200 sik nan 1C Figi kolore yo disponib sou sit entènèt.

 

Nan Fig. 6 (a), koub chaj-egzeyat echantiyon an NMTSb0 evidamman gen plizyè plato vòltaj ak etap, ki endike ke tranzisyon faz miltip soti nan egzagonal nan monoklinik ka rive nan estrikti nan kouch. Sepandan, pandan y ap glise interlayer nan kouch metal tranzisyon an rive, koub chaj-egzeyat la an jeneral relativman lis. Twa platfòm vòltaj ki pi wo a 3.00 V yo gen tandans flou. Pou NMTSb0, koub chaje a sitou divize an de pati: seksyon pant lan alantou 3.00-3.80 V ak seksyon plato long ki pi wo a 3.80 V. Sepandan, lè yo te prezante Sb, vòltaj inisyal la nan segman platfòm la te ogmante pi wo pase 4.00 V. Pou koub egzeyat la, plato long la anjeneral rive nan seri vòltaj 2.50-2.75. V. Ka aparans plato vòltaj la dwe atribiye a transfòmasyon faz O3 nan faz P3, pandan y ap segman pant la lè vòltaj la ogmante se reyaksyon solisyon solid ak estrikti P3 la. Figi 6(b) se yon konparezon pèfòmans sik nan NMTSbx (x=0, {{30}}.02, 0.0 4, 0.06) elektwòd nan yon dansite aktyèl 1C. Li enpòtan pou remake ke estabilite sikilasyon NMTSb0.04 materyèl katod se pi bon an, epi apeprè 70 pousan nan kapasite revèsib la ka kenbe apre 2{{95} }0 sik. Kontrèman, kapasite espesifik elektwòd NMTSb{{1{{1{107}}5}}1}} la dekonpoze trè vit, ak yon valè inisyal 122.8 mAh g-1, ki desann nan 51 mAh. g-1 apre 200 sik, epi sèlman 41.5 pousan nan kapasite espesifik la rete. Nan Fig. 6 (c, d), menm nan yon pousantaj trè wo nan 5C (1200 mA g-1), retansyon kapasite espesifik nan elektwòd NMTSb0.04 la se toujou 92.6 pousan (125.3 mAh g-1). Kapasite espesifik elektwòd NMTSb0 a se sèlman 106.7 mAh·g-1, ki pi wo pase lòt oksid ki te rapòte O3-kalite kouch. Kapasite espesifik egzeyat inisyal O3-Na(Ni1/3Mn1/3Fe1/3)0.95Al0.05O2 ki te prepare pa gwoup Yan nan yon pousantaj de 0.1C se 145.4 mAh·g-1. Epi apre 80 sik nan pousantaj 0.2C, kapasite espesifik revèsib la se 128.4 mAh·g-1. O3-NaNi0.5Mn0.5O2 gwoup rechèch Guo a prepare gen yon kapasite espesifik 80 mAh·g-1 nan seri vòltaj 2-4 V nan yon pousantaj 2C. Figi 6(e) prezante efikasite Coulombic batri Na-ion pandan monte bisiklèt kontinyèl nan 1C. Pami yo, distribisyon an efikasite Coulombic nan elektwòd NMTSb0.04 la se ki estab epi li gen tandans nan yon liy dwat, fondamantalman kenbe nan 98 pousan, ki tou endike ke estrikti kouch li yo pi estab. Sepandan, efikasite Coulombic nan elektwòd NMTSb0 la varye anpil apre 140 sik, e te gen yon gwo so lè li te tou pre 200 sik. Batri a reyini ak NMTSb0.04 apre 200 sik yo te demonte ak trete, epi yo te teste spectre XRD nan fèy elektwòd la, rezilta yo montre nan Figi S3. Pik difraksyon XRD nan moso poto NMTSb0.04 la pa t chanje anpil apre monte bisiklèt, sa ki endike ke chanjman faz irevokabl nan materyèl katod NMTSb0.04 la te siprime apre dopaj.

 

3 Konklizyon


Nan etid sa a, Na{{0}}.9Ni0.5-xMn0.3Ti{{{10}}.2SbxO2 (NMTSbx, x=0, 0.02, 0.04, 0.06), yon materyèl katod oksid kouch pou pil sodyòm-ion, te prepare pa yon metòd pratik eta solid. Patikil li yo konpoze de flak mikwo-nano-echèl ak epesè inifòm ak bor klè, ak gwosè grenn nan diminye apre Sb ranplase yon pati nan Ni. An menm tan an, dopaj la nan Sb lakòz fò delokalizasyon elèktron, ki diminye enèji nan tout sistèm nan epi li jwenn yon estrikti ki estab ki pi fezab nan sik chaj-egzeyat alontèm. Nan tès elèktrochimik nan seri 2.00-4.20 V, dopaj la nan Sb siprime tranzisyon an faz irevokabl nan materyèl la katod ak amelyore platfòm la vòltaj k ap travay. Lè yo chaje ak egzeyate nan pousantaj 1C, premye kapasite egzeyat espesifik NMTSb0.04 la se 135.2 mAh·g-1, ak pousantaj retansyon kapasite apre 200 sik se 70 pousan. Retansyon espesifik kapasite a ka rive jwenn 92.6 pousan (125.3 mAh·g-1) nan pousantaj 5C.

 

Referans


[1] MA A, YIN Z, WANG J,et al.

Al-doped NaNi1/3Mn1/3Fe1/3O2pou pèfòmans segondè nan pil ion sodyòm

Ionik, 2020,26(4):1797.

 

[2] ZHOU D, ZENG C, XIANG J,et al.

Revizyon sou materyèl katod ki baze sou Mn ak Fe ki baze sou kouch pou pil sodyòm-ion

Ionik, 2022,28(5): 2029.

 

[3] YAO HR, ZHENG L, XIN S,et al.

È-estabilite nan materyèl sodyòm ki baze sou kouch-oksid katod

Syans Lachin-Chimi, 2022,65(6):1076.

 

[4] LIU Z, ZHOU C, LIU J,et al.

Akor faz nan P2/O3-kalite katod oksid kouch pou pil ion sodyòmviayon senp wout ko-dopaj Li/F

Jounal Jeni Chimik, 2022,431: 134273.

 

[5] LI M, JAFTA CJ, GENG L,et al.

Korelasyon aktivite redox oksijèn anyon ak kòmande kation siwo myèl nan avyon an nan NaxNiyMn1-yO2katod

Rechèch avanse enèji ak dirabilite, 2022,3(7):2200027.

 

[6] LI J, LI H, HUANG Q,et al.

Etid sou mekanis nan enfliyans nan dopan sou pwopriyete yo nan materyèl katod nan pil sodyòm ion

Pwogrè nan Chimi, 2022,34(4):857.

 

[7] CHANJE YX, YU L, XING X,et al.

Estrateji sibstitisyon iyon nan katod oksid ki baze sou Manganèz pou pil ion sodyòm avanse ak pri ki ba.

Dosye chimik, 2022,6: 202200122.

 

[8] YIN YX, WANG PF, YOU Y,et al.

Yon O3-tip NaNi0.5Mn0.5O2katòd pou pil sodyòm-ion ak pèfòmans to amelyore ak estabilite monte bisiklèt

Journal of Materials Chemistry A, 2016,4: 17660.

 

[9] TAN L, WU Q, LIU Z,et al.

Ti-ranplase O3-kalite materyèl katod oksid kouch ak estabilite segondè-vòltaj pou pil sodyòm-ion

Jounal Syans koloyid ak entèfas, 2022,622: 1037.

 

[10] YUAN DD, WANG YX, CAO YL,et al.

Amelyore pèfòmans elektwochimik nan Fe-ranplase NaNi0.5Mn0.5O2materyèl katod pou pil sodyòm-ion

ACS Applied Materials Interfaces, 2015,16(7):8585.

 

[11] YUAN XG, GUO YJ, GAN L,et al.

Yon estrateji inivèsèl nan direksyon lè ki estab ak gwo pousantaj O3 kouch oksid katod pou batri Na-ion

Materyèl Fonksyonèl Avanse, 2022,32(17):2111466.

 

[12] ZHANG Q, WANG Z, LI X,et al.

Diminye fading vòltaj la ak sansiblite lè nan O3-tip NaNi0.4Mn0.4Cu0.1Ti0.1O2materyèl katodviaLa dopaj

Jounal Jeni Chimik, 2022,43: 133456.

 

[13] FIELDEN R, OBROVAC M N.

Ankèt sou NaNi axMn1-xO2(0 Mwens pase oswa egal axMwens pase oswa egal a 1) sistèm pou materyèl katod batri Na-ion

Journal of the Electrochemical Society, 2015,162(3):453.

 

[14] MATHIYALAGAN K, KARUPIAH K, PONNAIAH A,et al.

Wòl enpòtan nan sibstitisyon mayezyòm nan amelyore pèfòmans nan kouch O{0}}Na-Mn-Ni-Mg-O materyèl katod pou devlope pil sodyòm-ion

Jounal entènasyonal rechèch enèji, 2022,46: 10656.

 

[15] ZHOU C, YANG L, ZHOU C,et al.

Ko-sibstitisyon amelyore kapasite pousantaj la ak estabilize pèfòmans siklik nan O3-katòd NaNi.0.45-xMn0.25Ti0.3CoxO2pou depo sodyòm-ion nan vòltaj segondè

ACS Applied Materials & Interfaces, 2019,11(8):7906.

 

[16] CHENG Z, FAN XY, YU L,et al.

Yon estrateji rasyonèl bifaz adapte ki pèmèt katod segondè pèfòmans kouch pou pil sodyòm-ion.

Angewandte Chemie International Edition, 2022,61(19):17728.

 

[17] WALCZAK K, PLEWA A, GHICA C,et al.

NaMn0.2Fe0.2Co0.2Ni0.2Ti0.2O2segondè-entropi kouch oksid eksperimantal ak teyorik prèv nan pèfòmans elektwochimik segondè nan pil sodyòm

Energy Storage Materials, 2022, 47: 10656.

 

[18] DING Y, DING F, RONG X,et al.

Mg-dope kouch oksid katod pou Na-ion pil

Chinwa Fizik B, 2022,31(6):068201.

 

[19] HUANG Q, FENG Y, WANG L,et al.

Estrateji modulasyon estrikti pou siprime gwo vòltaj P3-O1 faz tranzisyon nan O3-NaMn(0.5)Ni(0.5)O2kouch katod

Jounal Jeni Chimik, 2022,431: 133454.

 

[20] WALCZAK K, PLEWA A, GHICA C,et al.

NaMn0.2Fe0.2Co0.2Ni0.2Ti0.2O2segondè-entropi oksid kouch: prèv eksperimantal ak teyorik nan pèfòmans elektwochimik segondè nan pil sodyòm

Materyèl Depo Enèji, 2022,47: 500.

 

[21] SONG T, CHEN L, GASTOL D,et al.

Estabilizasyon wo-vòltaj nan O3-kalite oksid kouch pou pil sodyòm-ion pa similtane fèblan doub modifikasyon

Chimi materyèl, 2022,34(9):4153.

 

[22] TANG W, SANVILLE E, HENKELMAN G.

Yon algorithm analiz Bader ki baze sou gri san patipri lasi

Journal of Physics Condensed Matter, 2009,21(8):084204.

 

[23] SANVILLE E, KENNY SD, SMITH R,et al.

Amelyore algorithm ki baze sou kadriyaj pou alokasyon chaj Bader

Journal of enfòmatik chimi, 2007,28(5):899.

 

[24] 韦帅, 胡朝浩, 钟燕, 等.

Sb掺杂LiBiO3电子结构的第一性原理计算

桂林电子科技大学学报, 2013, 33(4):339.

 

[25] XU Z, GUO X, WANG JZ,et al.

Limite efondreman oktaèd la nan katod NCM ki rich ityòm ak Manganèz nan direksyon siprime transfòmasyon estrikti.

Materyèl avanse enèji, 2022,12: 2201323.

 

[26] CHEN TR, SHENG T, WU ZG,et al.

Cu2 plisdoub-dope kouch-tinèl ibrid Na0.6Mn1-xCuxO2kòm yon katod nan batri sodyòm-ion ak estabilite estrikti ranfòse, pwopriyete elektwochimik, ak estabilite lè

ACS Applied Materials & Interfaces, 2018,12(10):10147.

 

[27] FENG T, LI L, SHI Q,et al.

Prèv pou enfliyans delokalizasyon polaron sou transpò elektrik nan LiNi0.4 plisxMn0.4-xCo0.2O2

Fizik Chimi Chimik Fizik, 2020,22(4): 2054.

 

[28] YADAV I, DUTTA S, PANDEY A,et al.

Evolisyon TiOx-SiOxnano-konpoze pandan recuit ultrathin fim oksid Titàn sou substra Si

Seramik Entènasyonal, 2020,46: 19935.

 

[29] SUN Z, DENG X, CHOI JJ,et al.

Silisyòm sifas pasivasyon pa lazè pwosesis yon Sol-Gel TiOxfim mens

ACS Applied Energy Materials, 2018,1(10):5474.

 

[30] YU L, XING XX, ZHANG SY,et al.

Kasyon dezòd O3-Na0.8Ni0.6Sb0.4O2katod pou pil sodyòm-ion wo-vòltaj

ACS Applied Materials & Interfaces, 2021,13(28):32948.

 

[31] KOUTHAMAN M, KANNAN K, ARJUNAN P,et al.

Kouch O3-tip Na9/10Kr1/2Fe1/2O2kòm nouvo katod pou rechargeable sodyòm-ion batri

Koloyid ak Sifas A: Aspè Fizikchimik ak Jeni, 2022,633: 127929.

 

[32] RYU HH, HAN G, YU TY,et al.

Amelyore estabilite monte bisiklèt O3-tip Na[Ni0.5Mn0.5]O2katod atravè Sn adisyon pou pil sodyòm-ion

Journal of Physical Chemistry C, 2021,125(12):6593.

 

[33] MENG X, ZHANG D, ZHAO Z,et al.

O3-NaNi(0.47)Zn(0.03)Mn(0.5)O2materyèl katod pou batri dirab Na-ion

Journal of Alloys and Compounds, 2021,887: 161366.

 

[34] ANANG DA, BHANGE DS, ALI B,et al.

Nouvo O3-tip Na ki estriktire nan kouch0.80[Fe0.40Co0.40Ti0.20]O2materyèl katod pou pil sodyòm-ion rechargeable

Materyèl (Basel), 2021,14(9):2363.

 

[35] LAMB J, MANTHIRAM A.

Sifas modifye Na(Ni0.3Fe0.4Mn0.3)O2katod ak lavi sik amelyore ak estabilite lè pou pil sodyòm-ion

ACS Applied Energy Materials, 2021,4(10):11735.

 

[36] CHEN C, HUANG W, LI Y,et al.

P2 / O3 bifaz Fe / Mn ki baze sou kouch oksid katod ak kapasite ultrahigh ak gwo sikilabilite pou pil ion sodyòm

Nano enèji, 2021,90: 106504.

 

[37] ZHENG YM, HUANG XB, MENG XM,et al.

Kwiv ak zikonyòm kodope O3-tip fè sodyòm ak oksid Manganèz kòm katod ki gen gwo kapasite ak lè ki estab nan cobalt/nikèl pou pil sodyòm-ion.

ACS Applied Materials & Interfaces, 2021,13(38):45528.

 

Enfòmasyon Siplemantè


Na-ion Battery Cathode Material

Fig. S1 HRTEM imaj NMT (a, b) ak NMTSb0.04 (c, d) ak enkadreman nan (b, d) ki montre imaj SEAD korespondan

 

Na-ion Battery Cathode Material

Fig. S2 (a) Ni2p, (b) Mn2p, (c) Ti2p, ak (d) Sb3d XPS spectre NMTSb0 ak NMTSb0.04

 

Na-ion Battery Cathode Material

Fig. S3 XRD modèl NMTSb0.04 kòm materyèl katod nan batri Na-ion apre 200 sik.

 

Tablo S1 rezilta ICP-AES nan O3-NMTSbx (x=0, 0.02, 0.04, 0.06) (Rapò esteyyometrik)

 

Na

Ni

Mn

Ti

Sb

NMTSb0

0.913

0.486

0.288

0.181

0

NMTSb0.02

0.924

0.471

0.284

0.186

0.023

NMTSb0.04

0.920

0.452

0.287

0.184

0.039

NMTSb0.06

0.929

0.435

0.279

0.184

0.061

 

Tablo S2 Paramèt lasi materyèl ak NMTSb0ak NMTSb0.04

 

a/nm

b/nm

c/nm

V/nm3

Rwp / pousan

Rp / pousan

NMTSb0

0.29812

0.29812

1.600487

0.1232

4.92

5.53

NMTSb0.04

0.29790

0.29790

1.608391

0.1236

5.65

6.32

Voye rechèch

whatsapp

Telefòn

Mel

Rechèch